| Steel & Alloy Material Type | Condition | Ultimate Tensile Strength (PSI) | 0.2% Yeild Strength (PSI) | Elongation (% In 2in.) | Reduction Of Area (%) | Hardness Brinell | Hardness Rockwell |
|---|---|---|---|---|---|---|---|
| XM-19 | Annealed | 100,000 | 55,000 | 35 | 55 | * | * |
| XM-19 | High Strength | 135,000 | 110,000 | 20 | 50 | 285-365 | * |
| K500 | Age Hardened | 140,000 | 100,000 | 20 | 40 | 265-346 | * |
| Alloy 20 | Annealed | 80,000 | 35,000 | 30 | 50 | 160 | * |
| Duplex 2205 | Annealed | 90,000 | 65,000 | 25 | * | 290 Max | * |
| 304 | Annealed | 75,000 | 30,000 | 30 | 40 | * | * |
| 304L | Annealed | 70,000 | 25,000 | 30 | 40 | * | * |
| 316 | Annealed | 75,000 | 30,000 | 30 | 40 | * | * |
| 316L | Annealed | 70,000 | 25,000 | 30 | 40 | * | * |
| 317 | Annealed | 75,000 | 30,000 | 30 | 40 | * | * |
| 317L | Annealed | 70,000 | 25,000 | 30 | 50 | * | * |
| PH 13-8 | H950 | 220,000 | 205,000 | 10 | 35 | 430 | C45 |
| H1000 | 205,000 | 190,000 | 10 | 40 | 400 | C43 | |
| H1050 | 185,000 | 175,000 | 11 | 45 | 380 | C41 | |
| H1100 | 150,000 | 135,000 | 14 | 50 | 313 | C34 | |
| H1150-M | 125,000 | 85,000 | 16 | 55 | 259 | C26 | |
| 15-5 PH | H900 | 190,000 | 170,000 | 6 | 15 | 388 | C40 |
| H1025 | 155,000 | 145,000 | 8 | 27 | 331 | C35 | |
| H1075 | 145,000 | 125,000 | 9 | 28 | 311 | C32 | |
| H1150 | 135,000 | 105,000 | 11 | 30 | 277 | C28 | |
| H1150-M | 115,000 | 75,000 | 14 | 35 | 255 | C24 | |
| 17-4 PH | H900 | 190,000 | 170,000 | 10 | 40 | 388 | C40 |
| H1025 | 155,000 | 145,000 | 12 | 45 | 331 | C35 | |
| H1075 | 145,000 | 125,000 | 13 | 45 | 311 | C32 | |
| H1150 | 135,000 | 105,000 | 16 | 50 | 277 | C28 | |
| H1150-M | 115,000 | 75,000 | 18 | 55 | 255 | C24 | |
| H1150-D | 125,000 | 105,000 | 16 | 50 | 255 | 24 | |
| 410 | T | 100,000 | 80,000 | 12 | 40 | * | * |
| H | 120,000 | 90,000 | 12 | 40 | * | * | |
| Annealed | 70,000 | 40,000 | 16 | 45 | * | * | |
| Class2 | 110,000 | 85,000 | 15 | 45 | 269 Max | * | |
| NACE MRO 175 | * | * | * | * | * | 22 HRC Max | |
| 416 | Annealed | * | * | * | * | 262 Max | * |
| Tempered | * | * | * | * | 248-302 | * | |